Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Transverse Bursting Strength Testing of Corrugated Medium Paper

Transverse bursting strength testing is a core quality control method for corrugating medium (corrugated base paper), measuring the maximum uniform hydraulic pressure the paper can withstand before rupture in accordance with ISO 2758, GB/T 454, and ASTM D774. This article explains the testing principle, applicable standards, specimen preparation, step-by-step test procedure, calculation of burst index, and practical applications in corrugated packaging production. It also provides answers to frequently asked questions to help packaging engineers, quality managers, and laboratory technicians obtain accurate and reproducible results.

Technical Overview

Corrugating medium is the fluted paper layered between the linerboards in corrugated board, typically produced in grammages of 80 g/m² to 200 g/m² and manufactured largely from recycled fibers or semi-chemical virgin pulp. Bursting strength is defined as the maximum uniformly distributed pressure, expressed in kilopascals (kPa), that can be applied perpendicularly to the paper surface through an elastic diaphragm before the sheet ruptures. It is one of the most widely specified strength properties for corrugated base paper because it reflects fiber bonding quality, formation uniformity, and the overall toughness of the sheet.

Although the rupture zone in a bursting test is subjected to a complex, roughly biaxial in-plane stress state, the test is conventionally designated as a transverse (cross-machine direction, CD) test because the cross direction governs failure initiation in machine-made paper. Due to fiber orientation during papermaking, CD strength is systematically lower than machine direction (MD) strength, so specimens are cut and marked with the transverse axis as the controlled test direction. This orientation-controlled convention ensures comparability between laboratories and between suppliers, and transverse bursting values are the figures quoted in trade specifications and acceptance contracts for corrugating medium.

The primary governing standards are ISO 2758 and GB/T 454 for paper, ISO 2759 and GB/T 1539 for heavier board grades, and ASTM D774/D774M as the North American equivalent. Conditioning of specimens is controlled by ISO 187 and GB/T 10739, while sampling follows ISO 186 and GB/T 450.

Testing Samples

Roll and Lot Samples

Samples are taken from production rolls or sheet lots in a manner representative of the entire lot, following the sampling principles of ISO 186 and GB/T 450. Samples must be free from visible defects such as wrinkles, holes, water marks, edge damage, and local contamination, and must be taken sufficiently far from roll ends and damaged outer layers. The machine direction of every sample must be clearly identified and marked before test pieces are cut, since correct transverse orientation is essential for a valid test.

Laboratory Test Pieces

Test pieces are cut to dimensions that fully cover the clamping circle of the bursting tester, typically at least 100 mm × 100 mm, with the transverse (CD) axis clearly marked. A minimum of 10 and preferably 20 valid test pieces are prepared, taken from positions distributed across the full width of the roll or sheet so that no two pieces represent the same location. All test pieces are conditioned to equilibrium in a standard atmosphere of (23 ± 1) °C and (50 ± 2) % relative humidity per ISO 187 or GB/T 10739 before testing, because moisture content has a strong influence on measured strength.

Verification Samples from Finished Board

For quality traceability, board plants may also prepare verification samples from the fluted layer of finished corrugated board, or perform burst testing on the combined board itself, to cross-check incoming medium quality against the properties declared by the paper supplier. In such cases, the origin and flute type of the sample must be documented in the test report.

Testing Items

The transverse bursting test program for corrugating medium typically includes the following measured and derived parameters:

  • Bursting strength: the maximum rupture pressure of the specimen, expressed in kPa (with legacy units such as kgf/cm² or psi reported only upon agreement).
  • Burst index: bursting strength divided by grammage, expressed in kPa·m²/g, which normalizes strength to basis weight and allows fair comparison between different grades.
  • Grammage (basis weight): determined separately per ISO 536 or GB/T 451.2 on the same conditioned sample, as it is required for index calculation.
  • Statistical evaluation: mean value, range, standard deviation, and coefficient of variation of all valid test pieces, together with the number of pieces tested and the number discarded.
  • Optional supporting determinations: thickness per ISO 534 and moisture content, when a more complete characterization of the lot is required.

Testing Methods

The test is performed on a Mullen-type bursting strength tester, either hydraulic (motor-driven piston displacing glycerin or water) or pneumatic. The conditioned test piece is securely clamped over a circular aperture of approximately 30.5 mm diameter for paper per ISO 2758 and GB/T 454, or approximately 31.5 mm for board per ISO 2759 and GB/T 1539. Fluid pressure is transmitted to the underside of the specimen through an elastic rubber diaphragm, which expands and applies a uniformly increasing pressure until the sheet ruptures; the maximum pressure at the moment of rupture is recorded as the bursting strength.

The general test procedure is as follows:

  • Verify and calibrate the apparatus before use: check pressure gauges or transducers against certified reference standards, inspect the diaphragm for aging and damage, verify clamp surface condition, and determine the diaphragm resistance correction as required by the standard.
  • Condition the test pieces to equilibrium at (23 ± 1) °C and (50 ± 2) % relative humidity, and handle them only by the edges to avoid contaminating or weakening the test area.
  • Clamp each test piece firmly with the marked transverse axis as the designated test direction, ensuring full contact with the clamp rings without slippage during the test.
  • Apply fluid at the constant delivery rate specified by the standard, approximately 95 mL/min for paper and approximately 170 mL/min for board, so that rupture occurs within the standard time window.
  • Record the maximum pressure indicated at rupture. Discard and replace any specimen that ruptures along the clamping line or slips during the test, and note the discard in the report.
  • Repeat the measurement on at least 10, preferably 20, valid test pieces taken from distributed positions.
  • Calculate the mean bursting strength, apply the diaphragm correction where applicable, and compute the burst index using the formula: burst index (kPa·m²/g) = mean bursting strength (kPa) ÷ grammage (g/m²).
  • Report the test standard used, tester type, conditioning atmosphere, specimen orientation, number of valid pieces, mean value, standard deviation, and burst index.

Key factors affecting accuracy include the moisture content of the specimen, grammage uniformity, diaphragm condition and calibration, clamping pressure, and strict control of specimen orientation. Participation in interlaboratory comparisons at accredited third-party laboratories is recommended to monitor ongoing precision.

Applications

Transverse bursting strength data for corrugating medium are used throughout the paper and packaging value chain:

  • Incoming quality control at corrugated board plants, verifying that delivered medium lots meet contractual strength specifications before processing.
  • Grade classification and product acceptance of corrugating medium against national and industry specifications, including the grade requirements of GB/T 6544.
  • Process and furnish optimization at paper mills, for example evaluating recycled fiber blending ratios, refining intensity, and chemical additives on sheet toughness.
  • Input data for corrugated box design, where burst strength complements edge crush and flat crush values in predicting box compression performance.
  • Supplier qualification, periodic audits, and trade settlement, providing an objective basis for acceptance or claims.
  • Research and development, failure analysis of damaged packaging, and technical support in quality disputes.

FAQ

What is transverse bursting strength of corrugated medium?

It is the maximum uniformly distributed pressure, in kPa, that a specimen of corrugating medium withstands before rupturing when the pressure is applied through an elastic diaphragm, with the specimen cut and marked so that the cross-machine (transverse) direction is the controlled test direction. Because CD strength is the weaker and therefore governing direction, transverse values are the conservative figures used in specifications.

Which standards apply to this test?

The main standards are ISO 2758 and GB/T 454 for paper, ISO 2759 and GB/T 1539 for heavier board grades, and ASTM D774/D774M as an equivalent method. Sampling and conditioning are covered by ISO 186/GB/T 450 and ISO 187/GB/T 10739 respectively, and grammage for index calculation is determined per ISO 536 or GB/T 451.2.

Why is the burst index reported in addition to bursting strength?

The burst index, calculated as bursting strength divided by grammage and expressed in kPa·m²/g, normalizes strength to basis weight. This allows meaningful comparison between lightweight and heavyweight grades and is the parameter commonly used in grade specifications and supplier benchmarking.

How many specimens should be tested?

At least 10 valid test pieces are required, and 20 is recommended, distributed across the width of the roll or lot. Specimens that rupture at the clamp line or slip must be discarded and replaced, and all discards must be documented.

What factors influence the test results?

Moisture content and conditioning atmosphere, grammage and formation uniformity, fiber orientation control, recycled fiber content, diaphragm age and calibration status, clamping pressure, and pressure delivery rate all significantly affect the measured value. Strict adherence to the specified atmosphere and apparatus verification is essential for reproducibility.

How does bursting strength relate to corrugated box performance?

Bursting strength reflects the toughness and internal bonding of the medium and contributes to the overall puncture and burst resistance of the finished board. It is used together with edge crush strength, flat crush strength, and board construction data in box performance models, and a low transverse burst value is an early warning of weak fiber bonding that can degrade box compression life.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing